A liner that fails at 40 % of expected life almost never fails because the steel grade was wrong. It fails because of something that was already inside the casting when it left the foundry. Buyers rarely get to see it, because most of these defects are internal - but some leave traces you can check on delivery.

1. Shrinkage porosity

What it is: the last metal to solidify contracts, and if there is no feed metal nearby, it leaves a sponge of voids. In a thick section like a mantle or a 5 tonne liner, the shrinkage sits in the thermal centre - the middle of the thickest part.

How it ends the part’s life: the porous zone has a fraction of the section’s load capacity. Under the cyclic loading of a cone crusher, a crack initiates at the void and grows outward until the liner breaks - often through the seating face, which writes off the concave as well.

How to spot it: you usually cannot, from outside. This is what ultrasonic testing is for. What you can check: whether the foundry poured through a riser sized for the section, and whether the riser was fed (a riser that froze before the casting is decorative). Ask for the UT record on the section behind the wear face for large parts.

Visible trace: a depression or “sink” on a thick face is a shrinkage indication that reached the surface. It is a legitimate reason to query a casting.

2. Gas porosity

What it is: gas trapped in the metal, from a damp mould, an unvented sand core, or a foam pattern that decomposed faster than the coating could vent it. It appears as round, smooth-walled holes, often just under the surface.

How it ends the part’s life: subsurface gas holes become the initiation site for spalling. On a blow bar, a cluster of gas holes behind the working face is a crack waiting for the first big lump.

How to spot it: on a machined face, look for pinholes. On a cast surface, look for “blowholes” - small craters. A few isolated pinholes on a non-critical surface are normal foundry practice and are not a defect claim; a cluster on the working face is.

Process control: dry sand, controlled moisture, vented cores. This is a discipline issue, not a design issue.

3. Sand inclusion / slag inclusion

What it is: moulding sand or slag that did not float out and is now embedded in the metal, usually near the bottom of the mould or behind a core.

How it ends the part’s life: the inclusion is a stress raiser and a discontinuity in the wear surface. It shows up as a pit that grows into a groove, and on jaw plates as a chipped tooth.

How to spot it: on a machined or ground surface, irregular dark patches that do not polish. On a fracture face after a failure, look for sand grains embedded in the metal - that is conclusive, and it is a foundry defect, not a service issue.

Process control: gating design and a clean pouring practice. Buyers can ask whether the foundry uses ceramic filters.

4. Hot tears (cracking during solidification)

What it is: a crack that opens while the casting is still hot, because a section is restrained by a colder part of the mould. It runs along grain boundaries and typically appears at a change of section or at a corner.

How it ends the part’s life: immediately, or at the first thermal cycle. A hot tear is a through-wall discontinuity.

How to spot it: a ragged, oxidised crack line - the surfaces are dark because the crack was open while hot. A crack that is bright and clean happened cold, during handling or machining, which is a different conversation. The oxidised appearance is the tell.

Process control: fillet radii at section changes, mould yield, and pouring temperature. This is where a foundry’s pattern-making discipline shows.

5. Coarse grain / overheated structure

What it is: the metal was poured too hot or held too long, and the grains grew. In manganese steel it is often paired with carbide precipitation at the grain boundaries if the quench was slow.

How it ends the part’s life: lower toughness, so the part chips rather than deforms. On a jaw plate this shows as teeth breaking off instead of wearing down.

How to spot it: only by metallography - which is why a photomicrograph with grain size belongs in the inspection package. On a fracture face, a coarse, shiny crystalline appearance is the visual clue.

Process control: recorded pour temperature and a logged water-toughening curve (we hold 1050-1100 °C and log the curve per batch).

6. Mismatch / dimensional drift

Not strictly a casting defect, but the one buyers notice first: bolt holes that do not line up, a seating face that rocks, a height that changes the closed-side setting.

How to spot it: trial-fit before the crusher is opened. On delivery, check bolt-hole pitch with a tape and check the seating face for rock on a surface plate if you have one. A liner that rocks will crack at the bolt holes.

The buyer’s triage

On delivery, before signing:

  1. Look for surface sinks or blowhole clusters on the working face - query them.
  2. Check bolt-hole pitch and seating face flatness, especially on a reorder.
  3. Check the heat number is stamped or on the shipping mark and matches the paperwork.
  4. If the part is large, ask for the UT record before it ships, not after it cracks.

Everything else is internal and needs either NDT or metallography. If a supplier cannot produce those on request for a large casting, the claim conversation after a failure will be short and one-sided.